) TEST REPORT FOR CEMENT TYPE OF CEM I 42.5R (TS EN 197-1)

TEST REPORT FOR CEMENT TYPE OF CEM I 42.5R (TS EN 197-1)
Sample Type
:
Taken Place
Sampling Date
CEMENT
Name of the Laboratory :
SONMEZ CEMENT LAB
:
Date of Report
:
29.9.2014
:
Report Number
:
Chemical Requirements
Test Results
Physical Requirements
3,15
2
3250
%
0,28
Silisium dioxide
%
20,30
Aluminium oxide (Al2O3)
%
4,09
Iron oxide (Fe2O3)
%
3,72
Calcium oxide (CaO)
%
63,73
Magnesium Oxide (MgO)
%
2,61
Potassium oxide (K2O)
%
0,76
Sodium oxide (Na2O)
%
0,12
Na2O eq
%
0,62
Sulfur Trioxide (SO3)
%
2,49
%
0,11
Chloride (Cl )
%
0,003
Prisms : 40 mm x 40 mm x 160 mm
Loss on Ignition (LOI)
%
1,60
Mixture : 1 Cement, 3 Sand, 1/2 Water
Free Lime (CaO)
%
1,10
Phosphore pentoxide (P2O5)
Potential
Mineralogical
Composition for
-
Spesific Gravity
( g/cm3 )
Insoluble Residue
Fineness
Spesific Surface
(cm /g)
0,200 mm Sieve Residue %
0,0
0,090 mm Sieve Residue %
0,2
0,045 mm Sieve Residue %
7,0
Setting Time (Vicat),
minutes
Initial (min)
140
Final (min)
215
Soundness (Le Chatelier), mm
1
STRENGTH REQUIREMENTS
Method EN 196-1
.
.
65,00
DAYS
Compressive Strength (N/mm2)
.
.
10,00
2
22,0
.
.
5,00
7
36,0
11,98
28
50,00
C3S ( 3 CaO SiO2 )
C2S ( 2 CaO SiO2 )
C3A ( 3 CaO Al2O3 )
.
.
.
C4AF ( 4 CaO Al2O3 Fe2O3 )
Quality and Assurance Manager
Quality and Assurance Engineer
Note:
*This test report belongs to the sample quoted above.
* All of analysis and tests were made according to TS EN 196.
*7 and 28 days comp. strength values will be declared according to written dates.
*This test report can't be copied partly without registered approval of SÖNMEZ CEMENT FACTORY.
Sönmez Çimento Yapı ve MadencilikSan. Tic. A.Ş.
Adana Yumurtalık Serbest Bölge Şubesi
Ceyhan / Adana / Türkiye
Tel: +90 322 634 21 70 | Faks: +90 322 999 33 22